Subject: Bending aluminum tube-2nd try
From: Paul
Date: 7/17/2000, 11:29 PM


Kent White wrote:

Paul,
I would attempt a bend only with the 1 3/8 OD 6061 T6 on a 4in radius to 90deg.
The trick is to do a partial and localized anneal with the torch on the inside of
the bend, encouraging the compression/shrinkage. Keeping the outside of the bend in
the T6 temper enables needed leverage and limits thinning. Remember that 650F is
the magic number, and that restraining the heat to one side of the tube will
involve rapid accurate heating and a heat fence. Temp. indicating crayons are
highly recommended along with a rapid water quench. Make the bend soon after, as
precipitation will begin to recover some of the strength as it ages.

Serrobend/bismuth filling just might do the trick, though swageloked ends and
either a water or mercury fill might do as well. Either way, use a bender and a
radius die, and re-anneal when the work-hardness threatens to wrinkle the inner
surface. It may take 2-3 annealings to make it.

It is a lot of fun to make a ball-pulling mandrel bender, but it just adds more
project to the project.

The 1.75" dia. 3" radius on a 180deg. return is probably a tad beyond any competent
shop mechanic. I would outsource mandrel-bent units from a Pines owner before I'd
recommend hugging a tar-baby like that.

It may be necessary to specify an easier bend, failing outsourcing.
Best of luck,
Kent
Kent White
www.tinmantech.com
TM Technologies, Tools and Methods for better Metalwork