Subject: Non rotary: welding 4130
From: Paul
Date: 2/6/2001, 11:37 PM


Stay away from the MIG. It will not deliver
 > > > aircraft quality welds.  TIG or Oxy/actyl are the two choices.
 > > > Jerry


 > I'm not a welding expert but would be interested in understanding
why MIG
 > won't provide quality workmanship on aircraft.  --  That's practically
all
I
 > see them use at the race track.  Everyone keeps saying the same thing,
but
 > no one ever explains why.  If you can de-mystify this, those of us who
 > aren't certified welders would appreciate it :-)
 >
 > Thanks,
 > Robin


The MIG (metallic Inert Gas) welder is just fine for non heat treatable
alloys and some aluminum. The rate of deposit and rate of cooling is very
fast. On low carbon steels this is a good weld, since there will be little
strength lost from rapid cooling. You can weld mild (low carbon) steel, and
drop it into cold water without causing a problem. This is not the case with
SAE 4130 and others. On thicker pieces the material should be warmed before
welding and covered, or dropped into a lime box to cool very slowly. On thin
wall tubing the problem is much worse. A breath of air can chill the weld
area quickly enough to install a near random selection of treated zones
across the weld area. If TIG (Tungsten Inert Gas) is being used, the joint
should be reheated and cooled very slowly. This can be done by covering the
joint with a drape of nonflammable material (not touching the work). The
reheat would include the weld and the tubing out from welded area for an inch
or inch and a half. Gas welding is so slow that a large area is heated just
doing the weld, so all that is left is the drape and slow cooling. This
returns the material to close to the as shipped, annealed condition.
Lynn E. Hanover


Technically, 4130 is supplied 'normalized' rather than annealed.  The
difference is subtle, but basically it is pretty hard to keep from getting
some extra
hardness and strength above annealed without going to heroic (silly) super
slow cooling rates.  Normailzed is stronger than truly annealed, but 4130 is
hard to actually anneal (dead soft) so it is normalized.  IIRC, 60ksi yield
in the normalized condition with 30% elongation to failure.   This is 4130's
big advantage - it will bend a LOT before breaking.  I like that in aircraft
structures.  Anything like a normal cooling rate will cause significant
hardening in 4130, with loss of ductility, but a gain in yield strength.
This again
supports  oxy-acetylene welding as you can easily play the torch over the
weld (a neutral flame provides heat and a reasonably effective blanket
against oxidation) and slowly draw it away to keep the cooling rate low.
Lynn is correct about drafts being pretty bad on thin walled tubing welds.
Weld indoors away from drafts. Esp in the winter.   Good safe 4130 welds
are not difficult with oxy-acetylene, but there are some do's and don't's.
Get and use FAA Pub. AC43.13-1A &2A (now 1B & 2B, I think)

Bill
Long EZ builder & pilot
mechanical engineer

 
The AirCraft Rotary Engine NewsLetter.              Powered by Linux.

http://home.earthlink.net/~rotaryeng/            http://www.linux.org