Subject: How to make Carbon fibre tubes water soluble plaster
From: Rotary Engine
Date: 2/16/2006, 4:49 PM
To: AA-me

   Autoclaving is not for the weak at heart. We use a lot of pressure and a
   lot of heat. Sometimes we even use argon because it has a better heat
   coefficient than air and doesn't oxidize parts and tooling under
   pressure.

   Vacuum bagging is sort of a poor middle ground between a wet layup
   and that
   nasty autoclave.

   eBay is an excellent resource for vacuum pumps (food sealers). I
   purchased
   one a couple of years ago on eBay for less than $20 including
   shipping and
   after cleaning the dried veggies and funk off of it was able to draw
   28.5inches of vacuum. That is exactly what we got on our central ($$$$)
   vacuum system here.

   Do I need to tell you what happened, I mean happens, if you draw
   resin into
   the kitchen pump? A little resin trap is a good idea. Again, mason jar
   (cans collapse, oops I keep showing my mistakes) with a tube in and
   a tube
   out.

   Hobby Lobby is another good source for layup materials. The polyester
   quilting batting works exactly like the breather material you buy from a
   composites supplier because it is exactly the same dang thing!

   I'm still looking for a poor man's peel ply. I think there is
   something at
   the fabric store that works. I just haven't found it yet. The peel
   ply we
   use is supposedly Teflon(tm) woven into a fabric. It has to breath some
   but won't stick to the resin. It looks like lingerie material
   although, I'm
   NO EXPERT on lingerie (whew!).

   The shiny blue tape you see the pros use to seal to the tool is
   designed for
   high temperatures. Clear packaging tape from the hardware store
   works just
   as well and is 10% the cost.

   We have a room full of bagging films some of which I'll never use again
   because they don't work. The best stuff is nylon but it doesn't
   stretch so
   we use it for flat layups, mostly. For the kitchen layup use laundry
   bags,
   painting drop cloth.

   Now, here's a hot tip. If you want to make a conformal bag, there is a
   product out there that works like a charm. It's called liquid latex
   and is
   also available from Hobby Lobby as Castin' Craft Mold builder. It's
   designed to be painted, rolled or poured onto something you need to
   replicate. In it's shipped form it's a little heavy but it can be
   thinned
   with a homemade solution of 50/50 ammonia and water. Use distilled water
   because if your tap water is a little hard you'll precipitate that
   out and
   it will cause lumps (ask me how I know that.)

   -Ben




   Great info Ben. If you have a chance write this all up or just edit what
   you have written and I will post it on the manifolds section of the web
   site under your name of course.


   Paul Lamar ...No rotor no motor.

Ben,

Are you the same Ben who is retired USAF F-15 driver?

What's your company website? I remember browsing it a while back and
seeing some interesting composite techniques. Are you still flying those
goodwill missions to Central America in your Viking?

Regards,

Gordon Arnaut
Ontario, Canada.



The Rotary Engine NewsLetter. Powered by Linux.
ACRE NL web site. http://www.rotaryeng.net
Copyright 1998-2006 All world wide rights reserved.