> Paul,
> I am working on the plane. Using Alumiprep, Alodine and the Variprime.
> The alumiprep look like it should, but the Alodine is failing to turn
> the parts gold toned. I just bought the bottle....
> Any ideas?
>
> --
> Blake C. Lewis
>
> The aluminum is not anodized is it?
> Did you acid etch it first before Alodine.
> What alloy is it?
>
> --
> Paul Lamar ...No rotor no motor.
>
> Blake, What's the temperature of the Alodine, I use Alumiprep also
> works great even in cool temperatures. However the Alodine needs to be
> warm at least 65 to 75 F to be active. Then it takes only 3 to 5
> minutes to coat the parts. Did you dilute the Alodine from the bottle?
> I believe the ratio is 2:1 Alodine to water. Matter of fact did some
> Alodining last night the temp of the mix was 68 when I started and 65
> when I finished. Parts came out just fine. Regards T.W.
I will check my temperatures next time. My shop is heated, but I
was venting cold air into it to help with the fumes. I was comfortable
in a long sleeve t-shirt though. It was 31F outside. The radiant floor
heat I installed in the shop is so comfortable. everything stays so
warm to the touch. I went ahead and painted everything with VariPrime.
--
Blake C. Lewis
I have had various shades of gold from just a dulling of the bright silver
left by the alumiprep to brown depending on how long I left the part exposed
to the alodine solution. Also old solution does not turn the part gold as
fast as new solution.
Joe berki
Limo EZ