This was a steep learning curve for me. I built a female mould teflon
lined and tried to use hardware store clear silicon rubber. The
silicone took weeks to fully cure if ever.
I went on the web and found one or two solutions. One mixed dish
washing detergent in a bucket of water and you were supposed to put
the silicon in that and massage it until it starting getting hard.
That sort of worked but it was imprecise.
Another suggested pure glycerin as a catalyst. As far as I can tell
that does not work at all.
Apparently there are two part silicone rubbers that do work but they
are really expensive. Apparently the colour is red.
I found red cured silicon rubber at McMaster one point five inches
thick relatively cheap at $60 for a six by six block 1.5 inches
thick.
It cut fine on my band saw.
So I made a pattern and printed it on label paper. The idea then is
to merely cut out the bumper rubber on the band saw.
Easier said then done. It toot several different programs on two
different operating system to achieve those printed labels :-) Then
it was a pain getting the sticky label off the label backing paper.
The trick here is put a bit of masking tape on the label side and it
is much easier to peel it off the backing.
I then cut hard wood blocks to check the back lash.
I am now moving ahead much faster :-)
Paul Lamar
About 40 yrs ago I working in a. wood-fiberboard manufacturing plant.
We used to resurface steel rollers in a sheet-conveyor system with what
they called "pourable rubber". I don't remember the brand name of the
stuff. It was a two-part system that created a somewhat transparent
substance that looked and felt like a stiff silicone rubber. Rubber
bonded very well to cast iron conveyor wheels. it held up well carrying
6' x 16' x 3/16 thick steel plates that were hot to the touch.
Components came in 1 gallon cans.
Robin Berglund's iphone
Check this out:
http://www.aeromarineproducts.com/silicone-mold-making.htm
There are lots of sources for two part silicone. I would recommend using a
bell jar to de-gas it before pouring it in your mold.
Steve Brazil
There is a difference. I am casting silicone parts in a closed mould.
I am not using it to make moulds that are exposed to air on the
outside of them.
If you have a little left over could you try it for me?
Make me a solid silicone rubber cylinder aprox. one inch
in diameter inch and a inch and a half long. Use a one inch
diameter steel or aluminium tube as a female mould.
Paul Lamar
The Rotary Engine News Letter. Powered by Linux. If you want off the
list PLEASE let me know and I will remove you. ACRE NL web site.
http://www.rotaryeng.net You Tube
http://tinyurl.com/beqqxas
Copyright 1998-2015 All world wide rights reserved.