This was a steep learning curve for me. I built a female
mould
teflon lined and tried to use hardware store clear silicon
rubber.
The silicone took weeks to fully cure if ever.
I went on the web and found one or two solutions. One mixed
dish
washing detergent in a bucket of water and you were supposed
to put
the silicon in that and massage it until it starting getting
hard.
That sort of worked but it was imprecise.
Another suggested pure glycerin as a catalyst. As far
as I can tell
that does not work at all.
Apparently there are two part silicone rubbers that do work
but they
are really expensive. Apparently the colour is red.
I found red cured silicon rubber at McMaster one point five
inches
thick relatively cheap at $60 for a six by six block 1.5
inches
thick.
It cut fine on my band saw.
So I made a pattern and printed it on label paper. The idea
then is
to merely cut out the bumper rubber on the band saw.
Easier said then done. It toot several different
programs on two
different operating system to achieve those printed labels
:-) Then
it was a pain getting the sticky label off the label backing
paper.
The trick here is put a bit of masking tape on the label
side and it
is much easier to peel it off the backing.
I then cut hard wood blocks to check the back lash.
I am now moving ahead much faster :-)
Paul Lamar
About 40 yrs ago I working in a. wood-fiberboard
manufacturing
plant. We used to resurface steel rollers in a
sheet-conveyor system
with what they called "pourable rubber". I don't remember
the brand
name of the stuff. It was a two-part system that
created a somewhat
transparent substance that looked and felt like a stiff
silicone
rubber. Rubber bonded very well to cast iron conveyor
wheels. it
held up well carrying 6' x 16' x 3/16 thick steel
plates that were
hot to the touch. Components came in 1 gallon cans.
Robin Berglund's iphone
Check this out:
http://www.aeromarineproducts.com/silicone-mold-making.htm
There are
lots of sources for two part silicone. I would
recommend using a
bell jar to de-gas it before pouring it in your mold.
Steve Brazil
There is a difference. I am casting silicone parts in
a closed
mould. I am not using it to make moulds that are exposed to
air on
the outside of them.
If you have a little left over could you try it for me? Make
me a
solid silicone rubber cylinder aprox. one inch in diameter
inch and a
inch and a half long. Use a one inch diameter steel or
aluminium
tube as a female mould.
Paul
Kit planes just had a good article on molding/mold making
silicon parts,
did you see it? Machined closed wood mold with pourable 2
part silicon?
Marc
Paul,
This is what you probably need. We used to seal fuel tanks and seaplane
floats.
We also used it as a coating for Tail rotor blades in high abrasive areas.
we just called it PRC but they have many different products.
PR-1547 High Hardness Potting and Molding Compound. -70°F (-57°C) to
300°F (149°C) – Durometer A 80
PR-1564 Low Viscosity, Medium Hardness Potting & Molding Compound -80°F
(-62°C) to 275°F (135°C) Durometer A 65
PR-1570 Medium Hardness Potting & Molding Compound. -80°F (-62°C) to
300°F (149°C) – Durometer A 75
PR-1574 High Hardness Potting & Molding Compound. -80°F (-62°C) to 300°F
(149°C) – Durometer A 90
PR-1590 Medium Hardness Potting & Molding Compound. -80°F (-62°C) to
300°F (149°C) – Durometer A 75
PR-1592 High Hardness Potting & Molding Compound. -70°F (-57°C) to 300°F
(149°C) – Durometer A 85
http://www.bergdahl.com/sealant/sealant-adhesives/pr-1590/
Barry Bordes
The durometer is way too high and the temperature is 100 degrees less
than Silicone.
Paul Lamar
The Rotary Engine News Letter. Powered by Linux.
If you want off the list PLEASE let me know and I will
remove you. ACRE NL web site.
http://www.rotaryeng.net
You Tube
http://tinyurl.com/beqqxas
Copyright 1998-2015 All world wide rights reserved.